gala gar SMART 200 MP Manuel Technique D'instructions page 23

Masquer les pouces Voir aussi pour SMART 200 MP:
Table des Matières

Publicité

Les langues disponibles

Les langues disponibles

SYMPTOM. ANOMALY.
THE WELDING START IS VERY
THE WELDING START IS VERY
THE WELDING START IS VERY
THE WELDING START IS VERY
AGGRESSIVE.
AGGRESSIVE.
AGGRESSIVE.
AGGRESSIVE.
THERE ARE MANY
THERE ARE MANY
THERE ARE MANY
THERE ARE MANY
PROJECTIONS.
PROJECTIONS.
PROJECTIONS.
PROJECTIONS.
SPECIALIZED PERSONNEL MUST CARRY OUT ANY WORK ON THE EQUIPMENT.
BOTH AT THE BEGINNING AND END OF A REPAIR CHECK THE EQUIPMENT INSULATION LEVELS.
DISCONNECT THE ELECTRONIC BOARDS WHEN MEASURING THE INSULATION.
BLOW THE INSIDE OF THE EQUIPMENT WITH COMPRESSED AIR.
The insulation-measuring device will have 500 V D.C. and will be applied to the following points of the circuit:
- Supply-Earth: Ra > 50 Mohms.
- Welding-Earth: Ra > 50 Mohms.
- Supply-Welding: Ra > 50 Mohms.
BEFORE TURNING THE EQUIPMENT ON, ENSURE THAT IT IS OFF LOAD.
DO NOT OPERATE THE ON/OFF SWITCH WITH AN ELECTRICAL LOAD CONNECTED TO THE
WELDING CONNECTORS.
SMART 200 MP
PROBABLE CAUSE.
Aluminium is being welded with a drawing
problem, which causes incorrect arc ignition as
the wire is slowed down on knocking against
the piece.
The wire length at onset of welding process is
too long.
POSSIBLE SOLUTION.
Examine the drawing process. Prevent the gun from making
"knots", keeping it in a straight line. The wire must not be
slowed down when it knocks against the piece
Correct arc end operation. Do not strike too long a final
wire length.